Incamake yihuse:

Amabuye ya mesh ashyigikira epoxy agomba guhanagura inshundura zishimangira, guhuza neza na plaque, no gukira kumuvuduko uhuye nubushyuhe bwuruganda. Umusaruro wubukonje ukenera chimie ikomeza guteza imbere mubihe bikonje, mugihe icyi cyangwa umusaruro wumurongo ukenera reaction igenzurwa kugirango epoxy itaza vuba. Hitamo sisitemu ukurikije ubushyuhe nyabwo bwamahugurwa, guhanagura mesh, igihe cyakazi, gukiza imyitwarire, imiterere yamabuye, numuvuduko wumurongo - ntabwo ukoresheje ubwiza cyangwa gukiza igihe wenyine.

Gushyigikira mesh bisa byoroshye bivuye hanze.

Icyapa kibuye cyahinduwe, mesh ya fiberglass gishyirwa inyuma, epoxy irakoreshwa, hanyuma nyuma yo gukiza icyapa gisubira mubikorwa.

Mubyukuri, iyi ni imwe mubikorwa aho uruganda rushobora gusubiramo urugendo rumwe buri munsi kandi rukabona ibisubizo bitandukanye cyane kuva Mutarama kugeza Kanama.

Mu gihe c'itumba, ibisigazwa birashobora kuba binini kandi bitinda gukira. Mesh fibre ikomeza kugaragara kuko epoxy itayitose neza. Icyapa gifata uduce twinshi kuruta uko byari byitezwe, kandi abakoresha batangira kwimura ibikoresho mbere yuko imbaraga zihagije zitera imbere.

Mu ci, ibinyuranye nabyo birashobora kubaho. Epoxy itemba neza mbere, ariko idirishya ryakazi riba rigufi. Igice kinini gitangira gushyuha muri kontineri, ibisigarira byiyongera mbere yuko igisate cyose gitwikirwa, cyangwa uruhande rumwe rwa mesh rwakira resin nyinshi kurenza urundi.

Igisubizo kigaragara ni ugushinja ubwiza.

Ariko viscosity nigice kimwe gusa cyigisubizo.

Ikibazo cyingirakamaro cyane ni ukumenya niba sisitemu yuzuye ya resin-ikomye yashizweho kugirango ikire byateganijwe ku bushyuhe aho umurongo winyuma ukorera.

Veropoxy kuri ubu itandukanya ibi bintu binyuze mubyeguriwe sisitemu ya epoxy sisitemu kubushyuhe buke nubushyuhe bwo hejuru mesh inyuma aho gufata ifumbire imwe nkumwaka wose wumwaka.

Amabuye ya mesh ashyigikira epoxy akoreshwa kumurongo wa marble mugihe cyo gukora uruganda

Niki Mesh Yinyuma?

Gushigikira amabuye ya mesh ni inzira yo gushimangira aho mesh ya fiberglass cyangwa ikindi gitambaro gishimangira gihujwe hejuru yinyuma yicyapa gisanzwe cyangwa cyubatswe.

Intego ntabwo ari ugukora ibisate byose muburyo bumwe.

Mesh na resin bikorana nkigice cyo gushimangira gishobora gufasha gutuza ibintu byoroshye, kugabanya ibyago byo gukwirakwira, no kunoza imikorere yizewe mugihe cyo gutunganya, gutwara, guhimba, no kuyishyiraho.

Kuki icyapa cyoroshye gikeneye imbaraga

Ibuye risanzwe ntirisanzwe.

Ibisate bibiri byaciwe kumurongo umwe birashobora kugira imipaka itandukanye yubutaka, imitsi, micro-crack, pore, ingano ya kirisiti, hamwe nihungabana ryimbere.

Ibikoresho byo gushushanya cyane birashobora kuba ingorabahizi cyane kuberako ibintu bigaragara abaguzi baha agaciro-kristu nini, imitsi itangaje, imyunyu ngugu, hamwe nuburyo budasanzwe - bishobora nanone guteza intege nke zaho.

Ubushakashatsi bwakozwe ku mabuye y’inyubako nini kandi zidasanzwe bwerekanye ko sisitemu ya epoxy ikozwe mu kirahure-fibre ishobora guhagarika ikwirakwizwa ry’imitsi no kunoza imyitwarire y’ubukanishi, nubwo imikorere ishimangira itandukana ukurikije ibuye, resin, sisitemu ya fibre, hamwe n’ubuziranenge bwa porogaramu.

Gushigikira mesh mubisanzwe bibaho mbere yo gusya

Kubice byinshi byerekana umusaruro, gushimangira bikorwa mbere yo gusya bwa nyuma.

Igice cyinyuma gikeneye gukira bihagije mbere yuko icyapa gisubira mugukora, gusya, gusya, cyangwa gutwara abantu.

Ibi bituma gukira igihe cyumusaruro, ntabwo ari laboratoire gusa.

Niki Cyiza Cyiza Gushyigikira Epoxy gikeneye gukora?

Epoxy yingirakamaro ya mesh ikenera ibintu byinshi icyarimwe.

Meza mesh ya fiberglass mesh

Ibisigarira bigomba kunyura no kuzenguruka fibre mesh aho kwicara hejuru yigitambara.

Gusiba neza bituma habaho guhuza fibre, epoxy, na substrate yamabuye.

Niba ahantu hanini cyera cyangwa humye hagumye kugaragara muri mesh, imbaraga zidahuye.

Ihambire hejuru yamabuye

Kunyunyuza fibre nziza ntibihagije niba epoxy idakurikiza neza icyapa.

Umukungugu, ubushuhe, ibisigara bitoboye, amavuta, ibishashara, ibikoresho byo kurekura, hamwe nuduce duto duto byose bishobora gukora intera idakomeye.

Komeza gukora igihe kirekire bihagije

Umukoresha akeneye igihe gihagije cyo gukwirakwiza epoxy hejuru yicyapa cyose no gutera inda mesh.

Sisitemu iva hagati yicyapa kinini irashobora gukora zone zikomeye kandi zidakomeye murwego rumwe rwo gushimangira.

Kiza byihuse kumurongo

Igihe cyakazi ntigishobora kurangira.

Iyo mesh imaze guhanagurwa neza hamwe na resin ihari, sisitemu igomba guteza imbere imbaraga zihagije zo kwimura icyapa binyuze mubikorwa byihuse.

Irinde gutemba gukabije

Niba ibisigazwa bitemba cyane mubihe byumusaruro nyirizina, birashobora kwimuka kure ya meshi, bikusanyiriza kumpande zicyapa, cyangwa bigatanga ikwirakwizwa rinini.

Komeza guhuzagurika binyuze mubihe bihinduka

Ibi nibisabwa cyane.

Ibisigarira bikora neza kuri 22 ° C birashobora kwitwara bitandukanye cyane kuri 10 ° C cyangwa 32 ° C.

Kuberiki Impeshyi nimbeho Gushyigikira bikeneye ingamba zitandukanye

Epoxy gukira ni ubushyuhe-bukabije.

Iyo ubushyuhe bugabanutse, epoxy idashidikanywaho muri rusange iba igaragara neza kandi imiti igabanya umuvuduko.

Iyo ubushyuhe buzamutse, muri rusange resin iba yoroshye gutemba, ariko reaction yo gukira nayo irihuta.

Ibi bitera ingaruka zinyuranye zibyara umusaruro.

Imiterere yumusaruro Imyitwarire Nkuru Ingaruka zisanzwe Icyo Uruganda rukeneye
Amahugurwa akonje Ubukonje buhanitse kandi buhoro buhoro Kuvomera nabi, gutinda gukira, gufata hakiri kare Ubushyuhe buke bukiza chimie
Ibihe biciriritse Kuringaniza gutembera no kwitwara Guhindura-guhinduranya ubushyuhe butandukanye Idirishya ryakazi rihamye kandi risubirwamo
Amahugurwa ashyushye Hasi ya viscosity yambere kandi byihuse Igihe gito cyakazi, kubyimba byihuse, gusaba kutaringaniye Kugenzura ubushyuhe bwo hejuru
Umurongo wumye Ubushyuhe bwihuse nyuma yo gusaba Gukiza imburagihe cyangwa iterambere rya gel ridahwanye Sisitemu yagenewe gukama-umurongo imiterere

Ingingo y'ingenzi iroroshye:

Igihe cy'itumba nimpeshyi bisaba kugenzura gukira gutandukanye nubwo mugihe intego yo kugaragara isa nimpapuro.

Gushyigikira Mesh Yimvura: Niki gihinduka mubushyuhe buke?

Umukozi ukoresha epoxy yubushyuhe buke kuri mesh amabuye asubira mumahugurwa akonje

Ibisigarira biba bigoye gukwirakwira

Nkuko epoxy idakize ikonje, ubusanzwe ubukonje burazamuka.

Uruziga cyangwa ikwirakwiza ikeneye imbaraga nyinshi. Resin inyura muri fiberglass gahoro gahoro, kandi fibre mesh irashobora kuguma yumye igice.

Ibi bigaragarira cyane cyane ku bisate binini aho uyikoresha akeneye gupfukirana metero kare.

Kwinjira mu ibuye birashobora kugabanuka

Gushyigikira mesh ntabwo gushingira gusa kumyenda.

Ibisigarira kandi bikenera imikoranire ihagije hamwe na pore, ubukana, nudusembwa duto hejuru yinyuma yicyapa.

Niba ibisigarira bibyibushye cyane, ibyo gutose no kwinjira hejuru birashobora kuba bike.

Igihe cyo gukira kiba kitateganijwe

Sisitemu isanzwe yubushyuhe irashobora gukomeza gukira mubihe bikonje, ariko "amaherezo" ntabwo aribisobanuro byerekana umusaruro.

Niba icyapa gikeneye inshuro ebyiri mbere yo gukora, sitasiyo yinyuma ihinduka icyuho.

Inganda noneho zitangire gufata ibyemezo bishobora guteza akaga nka:

  • kwimura ibisate mugihe ibisigarira bikiri icyatsi;
  • gutondekanya ibisate bishimangira hakiri kare;
  • Ongeraho Ikomeye;
  • ukoresheje ubushyuhe butagenzuwe; cyangwa
  • kwakira mesh yakize igice.

Izo shortcuts mubisanzwe zirema ibintu byinshi bihinduka.

Iyo Ubushyuhe Buke Mesh Gushyigikira Epoxy Bikora

Epoxy yo mu gihe cyitumba ntigomba gusa kuba formulaire isanzwe hamwe nibindi bikomeye byongewe muruganda.

Ubuvuzi bwa chimie ubwabwo bugomba kuba bwarateguwe kugirango bugumane ubukonje.

Veropoxy's Ubushyuhe buke Epoxy yo Kuringaniza Amabuye - 4090 / WBA25Q kuri ubu ihagaze hafi yumusaruro wa 10 ° C.

Sisitemu yatangajwe ikoresha:

  • 4090 / WBA25Q resin-gukomera;
  • 100: 25 kuvanga igipimo kuburemere;
  • 400-600 CPS ibishishwa;
  • hafi iminota 50 yo gukiza; na
  • hafi 10 ° C yasabye ubushyuhe bwakazi.

Igice cy'ingenzi ntabwo ari uko "iminota 50 iruta iminota 60."

Ingingo y'ingirakamaro ni uko sisitemu yashyizweho kugirango iteze imbere imikorere ikiza mugihe gikonje aho bisanzwe bisanzwe bishobora gukomera buhoro.

Ninde ukwiye gutekereza kuri sisitemu yo mu gihe cy'itumba?

Birumvikana iyo:

  • ubushyuhe bwamahugurwa buri gihe bwegera 10 ° C;
  • ibuye ubwaryo rirakonje nyuma yo kubika ijoro ryose;
  • Gushigikira mesh bibaho ahantu hadashyushye;
  • ibisate bigomba kwimurwa nyuma gato yo gushimangira;
  • gutinda gukiza imbeho bigabanya umurongo winjira; cyangwa
  • abakoresha bishyura intoki kugirango bakire buhoro.

Gushyigikira Impeshyi: Kuki Byihuta Ntabwo Buri gihe ari byiza

Umukozi ukoresha epoxy yubushyuhe bwo hejuru kuri mesh amabuye asubira kumurongo ushushe

Ikirere gishyushye gisa nkicyambere.

Epoxy itemba neza. Fiberglass ihinduka mucyo vuba. Abakoresha barashobora kwimura ibisigazwa hejuru yicyapa nimbaraga nke.

Hanyuma isaha itangira gukora kubarwanya.

Igihe cyo gukora kiba kigufi

Ubushyuhe bwo hejuru muri rusange bwihutisha epoxy reaction.

Ibisigarira birashobora gutangirira kumikorere ikora cyane ariko ikabyimba vuba kuruta uko byari byitezwe.

Ku gisate kinini, agace ka mbere karashobora guhanagurwa neza mugihe agace ka nyuma yakira resin yamaze gutangira kubaka ubwiza.

Ibice binini birashobora gushyuha byihuse

Epoxy gukira ni exothermic.

Imbaga nini ivanze mu ndobo yimbitse igumana ubushyuhe.

Ubushyuhe bwinshi bwagumishijwe burashobora kwihutisha reaction kurushaho.

Iyi ni imwe mu mpamvu abakoresha icyi rimwe na rimwe babona indobo ishyushye mugihe ibisigarira bimaze gukwirakwira ku gisate bikomeza gukora igihe kirekire.

Imirongo yumye yongeramo ubundi ubushyuhe burahinduka

Inganda zikoresha imirongo ishyushye cyangwa ifashwa nitanura ntigomba gutekereza gusa ubushyuhe bwicyumba ahubwo nubushyuhe bwatangijwe nyuma yo kubisabwa.

Sisitemu yo gukiza igomba kwihanganira urwo ruhererekane rutiriwe rwihuta.

Iyo Ubushyuhe Bwinshi Mesh Gushyigikira Epoxy Bikora

Ku mahugurwa ashyushye no gukama-umurongo, intego igenzurwa na reaction.

Epoxy iracyakenera gutemba neza no gutemba, ariko sisitemu yo gukiza igomba kubika umwanya uhagije wo gusaba kugirango urangize icyapa buri gihe.

Veropoxy's Ubushyuhe bwo hejuru butagira impumuro nziza Epoxy yo Kuringaniza Amabuye - 4090 / BCO25Q-14 kuri ubu yateguwe kuri 28 ° C + no kumisha-umurongo.

Ibisobanuro byatangajwe birimo:

  • 4090 / BCO25Q-14 sisitemu;
  • 100: 25 igipimo cya resin-kuri-gukomera kuburemere;
  • 400-600 CPS ibishishwa;
  • hafi iminota 60 yo gukira;
  • ubushyuhe bwo hejuru / 28 ° C + imiterere y'akazi; na
  • imikorere idahumura kubikorwa bikomeza umusaruro.

Ninde ukwiye gutekereza kuri sisitemu yo hejuru?

Birumvikana iyo:

  • ubushyuhe bwamahugurwa yubushyuhe burigihe burenga 28 ° C;
  • gushigikira mesh ikoresha amashyiga yumye cyangwa convoyeur zishyushye;
  • epoxy isanzwe itangira kubyimba mbere yuko porogaramu irangira;
  • ibisate binini bikenera igihe kinini;
  • abakoresha bavanga ibiro byinshi kuri buri cyiciro;
  • uruganda rukora imirongo ikomeza; cyangwa
  • akazi-igihe gihoraho kirenze umuvuduko mwinshi wo gukiza.

Impamvu CPS imwe 400-600 CPS idasobanura ibicuruzwa bimwe

Iri ni ryo somo ryingenzi ryabaguzi mu ngingo.

Sisitemu zombi za Veropoxy mesh-backing kuri ubu zitangaza hafi ya CPS 400-600.

Bombi kandi bakoresha igipimo cya 100: 25 kuburemere.

Nyamara kimwe cyakozwe hafi yumusaruro wa 10 ° C ikindi kigera kuri 28 ° C + cyangwa kumisha umurongo.

Ibyo bivuze ko itandukaniro nyaryo atari ubwiza gusa.

Chimie ikomera kandi yuzuye ikiza ikora imirimo myinshi yigihe.

Ibisobanuro Sisitemu y'itumba Impeshyi / Ubushyuhe bwo hejuru
Sisitemu 4090 / WBA25Q 4090 / BCO25Q-14
Ikoreshwa ryibanze Ubushyuhe bwo hasi mesh inyuma Ubushyuhe bwo hejuru / gukama-umurongo mesh inyuma
Ubushyuhe busabwa Hafi ya 10 ° C. 28 ° C + / ubushyuhe bwumurongo
Ikigereranyo cyo kuvanga 100: 25 kuburemere 100: 25 kuburemere
Byatangajwe neza 400-600 CPS 400-600 CPS
Byatangajwe igihe cyo gukiza Hafi yiminota 50 Hafi yiminota 60
Impamvu nyamukuru yo guhitamo Umuti wizewe mubihe bikonje Umuti ugenzurwa mubihe bishyushye

Abaguzi: Ntugahitemo icyi nimbeho mesh-backing epoxy ukoresheje viscosity wenyine. Sisitemu ebyiri zishobora gutangaza CPS hamwe nigipimo kimwe nyamara ikitwara muburyo butandukanye cyane kubera ko chimie ikomera hamwe numwirondoro wo gukiza byateguwe kubushyuhe butandukanye.

Mesh Wet-Out Nibyingenzi Kuruta Gupfuka Imyenda

Urushundura rushobora kugaragara "rutwikiriwe" mugihe rutaraterwa nabi.

Intego ni ya resin yohanagura fibre no gukora imikoranire ya hafi hagati yigitambara gishimangira nubuso bwamabuye.

Ni ubuhe buryo bukwiye busa

Iyo fiberglass itose neza hamwe na sisitemu ya epoxy isobanutse, fibre mubisanzwe iba mucyo kandi igaragara neza hamwe na resin layer.

Ibice byera byumye byera birashobora kwerekana inda zuzuye.

Inganda epoxy yubuyobozi ikoreshwa rya fiberglass nayo ishimangira gukwirakwiza ibisigazwa biva ahantu habi mu mwenda wumye no kuvanaho ibisigazwa byinshi mbere yo gusohora.

Ibisigarira bike cyane birema meshi yumye

Niba ingano yo gusaba ari mike cyane:

  • fibre iguma yumye igice;
  • guhuza amabuye bihinduka;
  • icyuho kiguma munsi ya mesh;
  • gushimangira byaho bigenda bigabanuka; na
  • gukuramo bishobora gutangirira ahantu hadahujwe.

Resin nyinshi ntabwo ihita iba nziza

Resin ikabije yongeramo ikiguzi nuburemere bitabaye ngombwa kunoza imbaraga.

Ibidengeri binini birashobora kandi gukiza umuti utaringaniye, uturere dukungahaye kuri resin, hamwe nubushyuhe budakenewe.

Intego ni yuzuye-yuzuye hamwe nubunini bugenzurwa.

Gutegura Ubuso Birashobora Guhitamo Niba Mesh igumaho

Ndetse epoxy nziza ntishobora guhuza kwizerwa no kwanduza.

Kuraho umukungugu

Gukata amabuye na kalibrasi bisiga umukungugu mwiza wamabuye hamwe nibisigara.

Niba ibyo bice bigumye kumurongo, epoxy irashobora guhuza umukungugu kuruta ibuye.

Igisubizo kirashobora kugaragara neza muburyo bwambere hanyuma ugakuramo mugihe cyo gukora.

Kugenzura ubuhehere

Ubuso bwamabuye butose burashobora kubangamira sisitemu nyinshi yo guhuza epoxy.

Niba ibisate bisize umurongo wo gukaraba mbere yo gusubira inyuma mesh, uruganda rugomba kwemeza ko ubuso bwinyuma bwageze kumiterere yumye mbere yo kubisaba.

Kuraho uduce duto duto

Amabuye yoroheje arashobora kugira ibinyampeke bidakomeye cyangwa amabuye y'agaciro ya flake hejuru yinyuma.

Guhambira inshundura kubintu bimaze gutandukana na plaque ntabwo bikemura ikibazo cyihishe inyuma.

Kuvanga Ikigereranyo Biracyafite akamaro mugihe cyizuba nimbeho

Ikibazo cy'ubushyuhe ntigikwiye gukemurwa muguhindura igipimo cyo kuvanga.

Sisitemu zombi za Veropoxy mesh-backing zerekana 100: 25 resin-to-gukomera kuburemere.

Iri gereranya rigomba kuguma rihamye keretse uwatanze isoko atanga ubundi buryo bwemewe.

Ntukongereho gukomera mu gihe cy'itumba

Ibikomeye cyane ntabwo bihindura neza epoxy isanzwe muri epoxy yubushyuhe buke.

Kuvanga kutagereranya bishobora kugabanya ubuvuzi bwiza kandi bigakora imiterere idahwitse.

Ntugabanye gukomera mu cyi

Mu buryo nk'ubwo, kugabanya gukomera ntabwo aribwo buryo bwiza bwo gukora sisitemu yo mu cyi gahoro.

Uburyo bwiza nugukoresha chimie ikiza igenewe kubyara ubushyuhe bwinshi.

Kubisobanuro byimbitse, reba Epoxy Resin Ivanga Ikigereranyo cyo gutunganya amabuye.

Ukuntu Viscosity igira ingaruka kumugongo

Gushyigikira mesh bikeneye kuringaniza.

Ibisigarira bigomba kuba binini bihagije kugirango bitose fibre hanyuma bigakwirakwira ku gisate, ariko bigenzurwa bihagije kuburyo bidahunga gusa urwego rukomeza.

Niba ubukonje buri hejuru

Umukoresha arashobora kubona:

  • gutwita nabi mesh;
  • uruziga rukomeye;
  • uduce twumye;
  • umwuka wafashwe cyane;
  • imbaraga nyinshi z'abakozi; na
  • gukwirakwiza resin.

Niba ubukonje buri hasi cyane

Ibibazo bishoboka harimo:

  • gutemba ku nkombe z'icyapa;
  • kwegeranya resin munsi yicyapa;
  • kwinjiza cyane mu ibuye rinini;
  • hasi yubaka; na
  • gukoresha ibikoresho byinshi.

Niyo mpamvu "kugenzurwa nubucucike buke" mubisanzwe ari ururimi rwingirakamaro kuruta "CPS yo hasi ishoboka."

Kubindi bisobanuro kuri iki cyemezo, reba Ubuyobozi Buke-Viscosity Epoxy Guide.

Intoki Mesh Gushyigikira vs Imirongo Yakozwe Yikora

Umusaruro wintoki ukeneye igihe cyakazi gikora

Abakozi b'intoki bakeneye igihe gihagije cyo:

  • shyira mesh;
  • kuvanga epoxy;
  • gusuka ibisigarira;
  • kuyikwirakwiza ku gisate;
  • akazi gakoreshwa ahantu humye;
  • gukuramo ibikoresho birenze; na
  • gukosora iminkanyari cyangwa ahantu humye.

Niba epoxy ihinduka vuba, ubwiza bwa porogaramu buterwa cyane numuvuduko wabakoresha.

Imirongo yikora ikeneye gusubirwamo

Imirongo yikora cyangwa igice cyikora irashobora gukoresha resin byihuse, ariko itangiza ikindi kintu gisabwa: igihe cyisubiramo.

Icyiciro kimwe ntigikwiye gutangira gucura iminota mike mbere yikindi kuko ubushyuhe bwibintu bwahindutse.

Kuri sisitemu zikoresha, suzuma:

  • gupima neza;
  • kuvanga ubudahwema;
  • ubushyuhe bwa resin;
  • umuvuduko w'umurongo;
  • umuvuduko wa roller;
  • guhuza ibiryo mesh;
  • ubushyuhe bw'itanura; na
  • gukoresha igihe nyuma yo gukira.

Ibisanzwe Bishyigikira Kunanirwa nicyo basanzwe basobanura

Ikibazo Cyakurikiranwe Impamvu zishoboka Ibyo Kugenzura Mbere
Ibishishwa bya mesh biva mu ibuye Ubuso bwanduye, gutose nabi, gukira kutuzuye Isuku yo hejuru, ubushuhe, gukwirakwiza resin no gukiza indwara
Ahantu humye humye hasigaye Ibihagije bidahagije cyangwa resin iragaragara cyane Ingano yo gusaba, viscosity na tekinike ya roller
Epoxy iguma yoroshye mugihe cy'itumba Ubushyuhe buri munsi yimiterere Ubushyuhe bwibidukikije, amabuye na resin
Epoxy geles vuba cyane mu cyi Ubushyuhe bwo hejuru cyangwa icyiciro kinini cya exothermic Ingano yubunini, ubushyuhe bwibintu hamwe na sisitemu ikomeye
Ibisigarira birangirira kumpande Sisitemu irenze urugero cyangwa sisitemu y'amazi menshi Ingano yo gusaba hamwe nubwiza bwubushyuhe bwumusaruro
Ibibyimba cyangwa ubusa munsi ya mesh Umwuka mubi, umuyaga wafashwe cyangwa kuzunguruka kutaringaniye Tekinike yo gusaba no guhuza imyenda
Ibice bitandukanye bikiza bitandukanye Kuvanga nabi cyangwa ubushyuhe butaringaniye Kuvanga uburinganire, igipimo nubushyuhe bwa plaque
Icyapa kimeneka nyuma yo gushyigikirwa Gushimangira bidahagije kumiterere yinenge Imiterere yamabuye, mesh ibisobanuro, resin itwikiriye nibisabwa bya mehaniki

Kuki "Kuma Gukoraho" Atari Igipimo Cyizewe

Icyapa gishobora kumva cyumye hejuru mugihe sisitemu yinyuma itigeze ikora imikorere ihagije yo gukora.

Ubushakashatsi busuzuma imbaraga z’amabuye y’inganda bwerekanye neza ko inganda rimwe na rimwe zisubiza ibisate ku musaruro zishingiye ku "gukama kwumye" aho kuba ibikenewe kugira ngo bikore.

Ibi bitera ibyago bitari ngombwa.

Sobanura ibipimo bifatika

Uruganda rugomba kumenya icyo icyapa gishimangira kigomba kubaho ubutaha:

  • guterura;
  • guhindukira;
  • ubwikorezi bw'amagare;
  • gutondeka;
  • kalibrasi;
  • gusya; cyangwa
  • ibihimbano.

Noneho impamyabumenyi yo gukiza igomba guhura nuwo mutwaro nyirizina.

Nigute Guhitamo Impeshyi vs Imvura Mesh Yinyuma Epoxy

Niba umusaruro wawe umeze… Shyira imbere… Kubera iki
Amahugurwa hafi ya 10 ° C. Ubushyuhe buke bukiza chimie Sisitemu isanzwe irashobora gukira buhoro buhoro kandi itose mesh nabi
Ibuye rikonje riva mububiko bwo hanze Reba ubushyuhe bwamabuye mbere yo kubisaba Igisate kirashobora kuguma gikonje kuruta umwuka wuruganda
Amahugurwa yo mu cyi hejuru ya 28 ° C. Kugenzura ubushyuhe bwo hejuru Ikomeza igihe cyakazi
Kuma ifuru cyangwa umurongo ushyushye Ubushyuhe bwo hejuru / umurongo-uhuza sisitemu Irinde gukira imburagihe mugihe cyo gushyushya
Intoki nini-plaque inyuma Umwanya uhagije wo gufungura Abakoresha bakeneye igihe cyuzuye
Umurongo uhoraho Batch-to-batch gukiza guhuzagurika Umuvuduko uhamye wumurongo uterwa nimyitwarire isubirwamo
Ibuye rinini cyane Kugenzura imigendekere no gukoresha resin Ibisigarira birenze birashobora kubura muri plaque
Ibuye ryoroshye cyane Kwemeza ubwinshi bwa mesh hamwe na sisitemu yo gushimangira byuzuye Epoxy yonyine ntabwo igena imbaraga zanyuma

Nigute Wapima Mesh Gushyigikira Epoxy Mbere yo Gutumiza Byinshi

Intambwe ya 1: Koresha ibuye ry'umusaruro nyirizina

Gerageza epoxy kuri granite imwe, marble, ibuye rya injeniyeri, cyangwa plaque zidasanzwe zitunganya uruganda.

Intambwe ya 2: Koresha mesh nyirizina

Ubucucike bwa mesh, imiterere ya fibre, hamwe nubuvuzi bwo hejuru birashobora kugira ingaruka kubisabwa no gutonyanga.

Intambwe ya 3: Gerageza ku bushyuhe bwibihe

Igihe cy'itumba kigomba kugeragezwa hafi yuburyo buteganijwe gutunganywa.

Ibicuruzwa byo mu cyi bigomba kugeragezwa kumiterere yubushyuhe bwo hejuru.

Intambwe ya 4: Andika igihe cyo gusaba

Gupima igihe cyo kuvanga kugeza icyapa cyose cyuzuye.

Intambwe ya 5: Andika ibyo ukoresha

Kurikirana garama cyangwa kilo kuri metero kare cyangwa icyapa.

Ibi nibyingenzi kugereranya igiciro cyumusaruro nyawo.

Intambwe ya 6: Reba mesh muburyo bugaragara

Kugenzura ahantu humye, ibituba, iminkanyari, guterura inkombe, hamwe no gukwirakwiza ibinini.

Intambwe 7: Emera gukira

Ntugabanye igihe cyo gukiza gusa kuberako ubuso bwumva bwumye.

Intambwe ya 8: Koresha icyapa ukoresheje uburyo nyabwo

Kuzamura, kuyimura, kuyihindura, no kuyisubiza mu musaruro ukurikije uko uruganda rusanzwe rukurikirana.

Intambwe 9: Gereranya ibisate byinshi

Icyitegererezo kimwe cyatsinze ntabwo gihagije kugirango yemererwe byinshi.

Guhindura amabuye bivuze ko sisitemu igomba kugenzurwa hejuru yicyapa gihagarariye.

Mesh Gushyigikira Epoxy Yabaguzi Kugenzura

Ikibazo Cyabatanga Impamvu bifite akamaro
Ni ubuhe bipimo by'ubushyuhe iyi igoye yagenewe? Kugena ibihe byo gukiza bikwiye
Ni ubuhe buvange buvanze ku bushyuhe bwavuzwe? Ifasha guhanura mesh yatose no gutemba
Ni ikihe gipimo cya resin-kuri-gukomera? Birasabwa gukira inshuro nyinshi
Ikigereranyo nuburemere cyangwa ingano? Irinde gukuramo amakosa
Idirishya ryingirakamaro rifite igihe kingana iki? Kumenya niba icyapa cyuzuye gishobora kurangira
Ni ryari icyapa gishobora gukemurwa neza? Byingirakamaro kuruta "gukiza igihe" kidasobanutse
Igicuruzwa kibereye imirongo yintoki cyangwa yikora? Umuvuduko wo gusaba uhindura umwirondoro ukenewe
Birakwiriye gukama-umurongo cyangwa gukiza ifuru? Nibyingenzi kuri sisitemu yubushyuhe ishyushye
Turashobora kugerageza icyitegererezo kumabuye yacu na mesh? Ikigeragezo nyacyo cyuruganda kigaragaza guhuza
Ni mu buhe buryo imikorere iri hagati yitsinda? Umusaruro uhoraho biterwa no gusubiramo

Amakosa asanzwe ashyigikira amakosa yo kwirinda

Gukoresha epoxy imwe umwaka wose utabanje kwipimisha ibihe

Niba ubushyuhe bwuruganda buhinduka cyane hagati yimbeho nimpeshyi, formula imwe ntishobora gutanga idirishya rimwe ryumwaka.

Ongeraho ibikomeye byiyongera mugihe cy'itumba

Ntabwo aribwo bugenzurwa nubushyuhe buke bwo gukiza chimie.

Kugabanya gukomera mu cyi

Ubu ntabwo aribwo buryo bwizewe bwo kongera igihe cyakazi.

Koresha inshundura hejuru yamabuye

Epoxy irashobora guhuza umwanda aho kuba icyapa.

Dufate ko kugaragara bigaragara bisobanura byuzuye

Ibisigarira bigomba gutera inshundura meshi no gukora imikoranire yizewe nibuye.

Kwimura ibisate bikimara kumva byumye

Gukoraho-kumisha ntabwo byerekana imbaraga zihagije zo gukora.

Kwirengagiza ubushyuhe bwamabuye

Icyapa ubwacyo kirashobora gukonja cyane cyangwa gushyuha kuruta umwuka wamahugurwa.

Kugereranya epoxy gusa kubiciro kuri kilo

Ibicuruzwa bihendutse bitwara resin nyinshi, bidindiza umurongo, cyangwa gukora rework birashobora kuba bihenze kumurongo warangiye.

Icyifuzo: Hitamo Sisitemu yo gukiza hafi yigihe cyumusaruro

Epoxy nziza ya mesh-nziza ntabwo ari ibicuruzwa bifite umuti wihuse cyangwa ubukonje buke.

Nibwo buryo butuma uruganda rutose neza meshi, rugakomeza guhuza kwizerwa, kandi rukagera ku mbaraga zo gufata neza ubushyuhe nyabwo.

Niba uruganda rukora hafi ya 10 ° C mugihe cy'itumba, shyira imbere ubushyuhe buke bwo gukiza imiti.

Niba umusaruro uhora hejuru ya 28 ° C cyangwa ugakoresha umurongo wumye, shyira imbere ubushyuhe bwo hejuru.

Niba umubare umwe wijimye ugaragara kubicuruzwa byombi, ntukibwire ko bihinduka.

Gereranya ibyuzuye byuzuye-bigoye, igihe cyakazi cyingirakamaro, gukiza imyitwarire, mesh yatose, ubushyuhe bwa plaque, umuvuduko wumurongo, nibisubizo nyabyo.

Niba kandi ibuye ryoroshye bidasanzwe, ryacitse cyane, cyangwa ryubatswe muburyo butandukanye, fata inyuma ya mesh nka sisitemu yuzuye yo gushimangira - ntabwo ari kugura gusa.

Ibibazo Bikunze Kubazwa Kubijyanye na Kibuye Mesh Gushyigikira Epoxy

1. Ni ubuhe bwoko bwa epoxy bwiza kuruta gufata amabuye mesh?

Epoxy nziza iterwa nubushyuhe bwamahugurwa, imiterere yamabuye, ubwoko bwa mesh, umuvuduko wumusaruro, nibisabwa gukira. Uruganda rwitumba rushobora gukenera sisitemu yo gukiza ubushyuhe buke, mugihe amahugurwa ashyushye cyangwa umurongo wumye ukenera ubushyuhe bwo hejuru. Gutonyanga neza mesh, kwizirika amabuye yizewe, nigihe gihagije cyakazi ni ngombwa kuruta guhitamo ubwiza bwonyine.

2. Ese epoxy imwe yinyuma ishobora gukoreshwa mugihe cyizuba nimbeho?

Rimwe na rimwe, ariko ntibigomba gufatwa. Ubushyuhe bunini bwibihe bigira ingaruka kuri epoxy viscosity no gukiza umuvuduko. Inganda zikora nka 10 ° C mu gihe cyizuba no hejuru ya 28 ° C mu cyi zishobora kungukirwa na sisitemu zitandukanye zo gukiza zagenewe ubwo bushyuhe.

3. Kuki mesh ushyigikira epoxy ikiza buhoro mugihe cy'itumba?

Ubushyuhe buke muri rusange bwongera ubwiza bwa epoxy kandi butinda reaction-gukomera. Niba formulaire itagenewe ibihe bikonje, guhindagura mesh hamwe niterambere ryimbaraga birashobora kuba buhoro cyane kubikorwa bisanzwe.

4. Kuki epoxy gel yihuta cyane mugihe cyizuba gishyigikiwe?

Ubushyuhe bwo hejuru bwihutisha gukira epoxy. Ibice binini bivanze birashobora kandi kugumana ubushyuhe bwa exothermic, bigatuma reaction yihuta imbere yivanga. Koresha ubushyuhe bukwiranye na chimie, ugenzure ingano yicyiciro, kandi ukurikirane ubushyuhe bwa resin na slab aho guhindura igipimo cyihariye cyo kuvanga.

5. Nigute uruganda rwamabuye rugomba kugerageza mesh inyuma ya epoxy mbere yo gutumiza byinshi?

Koresha ibuye ryakozwe na meshi, gerageza munsi yubushyuhe bwibihe byerekana, wandike resin ikoreshwa nigihe cyakazi cyakazi, genzura fibre yuzuye, wemererwe gukira, hanyuma ukoreshe icyapa ukoresheje uburyo busanzwe bwo gukora. Gereranya ibisate byinshi mbere yo kwemeza itangwa ryinshi.

Nigute ushobora kugumisha amabuye meshi mugihe cyizuba nimbeho

Gushimangira mesh kwizerwa biterwa no guhuza resin itemba no gukiza chimie mubidukikije nyabyo. Ibihe byimbeho byongera ubukonje no gutinda buhoro, mugihe ubushyuhe bwimpeshyi butezimbere ubwambere ariko bigabanya idirishya ryakazi. Sisitemu iboneye igomba guhanagura neza meshi, guhuza hejuru yamabuye asukuye, kandi igateza imbere imbaraga ziteganijwe zidateganijwe guhatira abashoramari kwishyura ubushyuhe hamwe no kuvanga bitagereranijwe cyangwa gushyuha bitagenzuwe.

Hitamo gukomera hafi yubushyuhe bwuruganda

Niba umusaruro wubukonje wegereye 10 ° C, koresha chimie yagenewe gukira neza mubushyuhe buke. Niba umusaruro wimpeshyi urenze 28 ° C cyangwa ugakoresha imirongo yumye, koresha sisitemu yubushyuhe bwo hejuru ibika igihe gihagije cyo gukora kugirango yinjizwe neza.

Huza inzira nuburyo bwo gukora

Amahugurwa akonje:
shyira imbere ubushyuhe buke bwo gukiza chimie kandi ugenzure neza-ibuye rikonje.

Umusaruro ushushe:
kurinda idirishya ryingirakamaro kandi wirinde kurenza urugero.

Umusaruro wumye:
koresha formulaire yagenewe gukira kugenzurwa nubushyuhe bwo hejuru.

Gushyigikira intoki:
menya neza ko abakoresha bafite igihe gihagije cyo gufungura inda yuzuye.

Ibuye ryoroshye cyangwa ridasanzwe:
suzuma ubwinshi bwa mesh, sisitemu ya epoxy, inenge yamabuye, hamwe nibisabwa hamwe.

Ntugacire urubanza gushimangira kugaragara-gukama

Ubuso bwumva bwumye ntabwo buhita bwitegura guterura, guhindukira, gusya, cyangwa gutwara. Sobanura ibyangombwa bisabwa kugirango ukemure kandi ubyemeze ku bisate nyabyo. Igihe cyiza cyo gukiza nigihe gikenewe kugirango ugere ku ntambwe ikurikiraho itekanye - ntabwo ari igihe gusa ubuso buhagaritse kumva bworoshye.

Ni iki abaguzi bagomba kugereranya hagati yabatanga isoko?

Gereranya ubushyuhe bwubushyuhe, kuvangavanga kwijimye, igihe cyakazi, gukiza imyitwarire, gusabwa ingano yicyiciro, guhanagura mesh, gufatisha amabuye, umwirondoro wimpumuro, guhuza umurongo wumurongo, gukoresha resin, no guhuza ibyiciro. Noneho gerageza sisitemu ngufi ukoresheje ibuye ryawe bwite, mesh, abakoresha, nibihe byumusaruro.

Icyifuzo gifatika

Niba gukira kwimbeho bitinze cyane, hindukira kuri chimie yubushyuhe buke aho kongeramo ibintu bikomeye. Niba icyi cya resin geles mbere yuko icyapa gitose, koresha sisitemu yubushyuhe bwo hejuru hamwe na reaction igenzurwa aho kugabanya gukomera. Niba ibishishwa bya meshi, genzura imyiteguro yubuso, bitose, kandi ukire mbere yo gushinja fiberglass. Niba kandi icyapa cyoroshye kiracika nyuma yo gushyigikirwa, suzuma igishushanyo mbonera cyuzuye aho gutekereza ko epoxy yonyine izakemura ikibazo.

Ukeneye Mesh Yinyuma Epoxy Kubushuhe Bwukuri Bwubushuhe?

Ubwoko bwamabuye, fiberglass mesh, ubushyuhe bwamahugurwa, ubushyuhe bwibisate, umuvuduko wumurongo, uburyo bwo gukiza, hamwe na gahunda yo gukora byose bigira ingaruka kumikorere ya mesh-backing. Gerageza sisitemu yuzuye mubihe byimbeho nizuba mbere yo kwemeza umusaruro mwinshi.


Shakisha Veropoxy Mesh Gushyigikira Epoxy Sisitemu

Reba

  1. A. A. Pazeto, P. M. Amaral, J. R. Pinheiro na A. B. Paraguassú.
    Ingaruka za Fibre Fibre-Gushimangira Kuburyo bwa Mechanical of Coarse Grained Grained Building Stone.
    Ikigo cy’ikoranabuhanga ry’amabuye y'agaciro na kaminuza ya Lisbonne.
    Ibikoresho byo kubaka no kubaka, Vol. 155, 2017, imp. 79–87.
  2. A. A. Pazeto, P. M. Amaral na R. L. Arcanjo.
    Isesengura ryimikorere yuburyo busanzwe bwo gushimangira Amabuye yo kubaka "Exotic" Ukurikije Ibisabwa Tekiniki Yubu.
    Ikigo cy’ikoranabuhanga ry’amabuye y'agaciro na IDMEC, kaminuza ya Lisbonne.
    Ikinyamakuru mpuzamahanga cy’ubukanishi n'ubumenyi bw'amabuye y'agaciro, Vol. 135, 2020, ingingo ya 104507.
  3. CYIZA SYSTEM Abakozi ba tekinike.
    Gukoresha imyenda ya Fiberglass na Tape.
    Gougeon Brothers, Inc.
    WEST SYSTEM Epoxy Technical Resources.
  4. CYIZA SYSTEM Abakozi ba tekinike.
    Epoxy Chemistry Shingiro: Gusobanukirwa Igihe Cyiza nubushyuhe.
    Gougeon Brothers, Inc.
    WEST SYSTEM Epoxy Technical Resources.
  5. CYIZA SYSTEM Abakozi ba tekinike.
    CYIZA SYSTEM Umukoresha Igitabo & Ubuyobozi.
    Gougeon Brothers, Inc.
    SYSTEM YIZA CYANE.
  6. Komite mpuzamahanga ya ASTM C18 ku Kibuye.
    ASTM C880 / C880M-25 - Uburyo Bwipimisha Uburyo Bwimbaraga Zimbaraga Zimbaraga Zibuye.
    ASTM Mpuzamahanga.
    Igitabo ngarukamwaka cyibipimo bya ASTM, Vol. 04.07.
  7. Komite mpuzamahanga ya ASTM C18 ku Kibuye.
    ASTM C99 / C99M - Uburyo busanzwe bwo gupima Modulus yo guturika kwamabuye.
    ASTM Mpuzamahanga.
    Igitabo ngarukamwaka cyibipimo bya ASTM, Vol. 04.07.
  8. Charles Selwitz.
    Epoxy isubira mu kubungabunga amabuye.