Incamake yihuse:
Mbere yo gutumiza byinshi kuri epoxy resin, uruganda rwamabuye rugomba kugerageza ibicuruzwa kuri marble nyayo, granite, onigisi, cyangwa ibuye ryakozwe mubihe byakozwe neza. Reba kuvanga imyitwarire, ubwiza, igihe cyakazi, gukira, kwinjira, gufatira, guhindura amabara, gukora neza, gukoresha resin, no guhuza ibyiciro. Ntukemere epoxy kuko icyitegererezo kimwe "gisa neza." Sobanura ibipimo / gutsindwa mbere, gerageza ibyapa byinshi byerekana, gereranya nibikorwa byawe byubu, kandi urebe imikorere mugihe cy'ubushyuhe n'impeshyi.
Kugura inganda epoxy resin bitandukanye no kugura igice cyarangiye.
Utanga ibicuruzwa arashobora kohereza ibicuruzwa bikosowe muburyo bwa tekiniki, ariko icyo gicuruzwa kirashobora kuba kibi kubuye ryibuye, ubushyuhe bwumusaruro wawe, urutonde rwa polishinge yawe, abakoresha bawe, cyangwa igihe cyinzira yawe.
Niyo mpamvu uruganda rwamabuye rutagomba na rimwe gufata icyitegererezo nkimpano nto yo kwamamaza.
Icyitegererezo ni igikoresho cyujuje ibyangombwa.
Intego ntabwo ari ugusubiza gusa:
“Iyi epoxy irakora?”
Ikibazo cyiza ni:
Ati: "Iyi epoxy irashobora gutanga inshuro nyinshi icyapa cyarangiye mu bihe byakozwe neza ku giciro cyemewe mu bucuruzi?"
Itandukaniro rifite akamaro.
Ibisigarira birashobora kwinjira neza ariko bigatwara ibintu byinshi. Undi arashobora gukira vuba ariko ugasiga abakora umwanya muto wakazi. Sisitemu isobanutse neza irashobora gukora halos yijimye kuri marble yera yera. Igiti gikomeye gishobora kugorana. Icyitegererezo kirashobora gukora neza kuri 24 ° C ariko kigenda gahoro cyane mugihe cyimbeho cyangwa ntigishobora guhinduka mugihe cyizuba.
Ibiriho bya Veropoxy amabuye ya epoxy ibicuruzwa portfolio iragaragaza ubu buryo bwihariye bwo gukoresha, hamwe na sisitemu zitandukanye za granite, marble, ibuye ryera, inyuma ya mesh, infashanyo ya vacuum, ibuye ryigiciro cyinshi, nibindi bintu byo gutunganya.
Amapaji menshi yibicuruzwa bya Veropoxy nayo atanga ingero byumwihariko kuburyo inganda zishobora gusuzuma imikorere mbere yo kugura byinshi. Nibyo rwose uburyo amasoko yabigize umwuga agomba kuyakoresha.
Impamvu Icyitegererezo Cyipimisha Mbere Yumubare Winshi wa Epoxy
Urupapuro rwa tekiniki ya epoxy irakubwira uko ibicuruzwa bitwara mubihe byasobanuwe.
Uruganda rwawe ntirushobora gukora muri ibyo bihe.
Ibuye risanzwe rirahinduka
Ibuye risanzwe ntabwo ari ikibaho gisanzwe.
Ibisate bibiri bya marble biva muri kariyeri imwe birashobora gutandukana muri:
- ubwoba;
- ubwinshi bwa micro-crack;
- imiterere y'amabuye y'agaciro;
- kwinjiza amazi;
- gusobanuka;
- Ubuso bukabije;
- ibara ryerekana amabara; na
- intege nke imbere.
Epoxy ikora neza kumabuye imwe irashobora gutanga ibisubizo bitandukanye kurindi.
Umusaruro wawe uhindura ibisubizo
Imikorere irashobora kandi guhinduka hamwe na:
- ubushyuhe bw'amahugurwa;
- ubushyuhe bw'amabuye;
- kuvanga ibikoresho;
- ingano y'icyiciro;
- imfashanyigisho cyangwa iyikora;
- umuvuduko wa vacuum;
- mesh;
- igihe cyo gukiza;
- gusya; na
- gusya.
Niyo mpanvu abatanga laboratoire bagomba guhitamo urutonde - ntibisimbuze ikigeragezo cyawe.
Abaguzi: Ikizamini cyingirakamaro cyane epoxy nticyizamini cya laboratoire igoye cyane. Nibizamini byerekana imiterere izagaragaza niba ibicuruzwa byatsinze cyangwa binaniwe kumurongo wawe.
Sobanura Pass / Kunanirwa Ibipimo Mbere yuko Icyitegererezo kigera
Iri ni rimwe mu itandukaniro rinini hagati yubushobozi bwumwuga no kwipimisha bisanzwe.
Ntukoreshe epoxy mbere hanyuma uhitemo nyuma niba "ubikunda."
Sobanura ibipimo byemewe mbere yo kwipimisha.
Tangira nibikorwa byawe byubu
Niba uruganda rwawe rumaze gukoresha epoxy yemewe, andika uko ibicuruzwa bikora.
Urugero:
- gukoresha resin kuri metero kare;
- impuzandengo y'akazi;
- igihe cyo gukiza;
- umubare w'ibyapa byasanwe kuri buri cyiciro;
- kwanga igipimo;
- ibisubizo;
- gusana ibiboneka;
- igihe cyo gufata mesh; na
- igiciro kuri buri cyapa cyarangiye.
Epoxy nshya igomba kugereranwa niyi shingiro aho gusuzumwa mu bwigunge.
Hitamo ibitagenze neza bitemewe
Kuri marble yera, halo igaragara yumuhondo irashobora kwangwa byikora.
Kuri granite yumukara, gucamo kutuzuye bishobora kuba ngombwa.
Kubishyigikira mesh, gukuramo nyuma yo gukora birashobora kutemerwa.
Kuri vacuum infusion, ubujyakuzimu budahagije burashobora gutuma igeragezwa ryose ridafite intego.
Ikizamini 1: Ongera usuzume inyandiko za tekiniki mbere yo gufungura icyitegererezo
Icyitegererezo kigomba kugera hamwe namakuru ahagije yo kugikoresha neza.
Subiramo TDS
Urupapuro rwa tekiniki rugomba gusobanura ibipimo bijyanye n'umusaruro, nka:
- ibiranga ibicuruzwa;
- gusaba;
- A: B igipimo cyo kuvanga;
- niba igipimo kiri muburemere cyangwa ingano;
- ubwiza;
- ubushyuhe busabwa;
- igihe cyo gukora cyangwa gukiza;
- uburyo bwo kubika; na
- amabwiriza yo gusaba.
Subiramo SDS
Urupapuro rwumutekano ntabwo ari inyandiko yimikorere.
Itanga amakuru ajyanye n’ibyago, gutunganya, kubika, kugenzura, PPE, ubufasha bwambere, gutwara, no kujugunya.
Umuguzi ukomeye winganda agomba kwitega ibyangombwa bya tekiniki n'umutekano.
Reba niba ibizamini bisobanuwe
Agaciro ka viscosity nka "500 CPS" bisobanura bike cyane mugihe utanga isoko atavuze cyangwa ngo agenzure imiterere yapimwe.
Mu buryo nk'ubwo, "gukiza iminota 60" ntabwo byuzuye keretse usobanukiwe n'ubushyuhe n'icyo gukiza intambwe uwatanze asobanura.
Ikizamini 2: Emeza ibicuruzwa nibiranga
Mbere yo kuvanga ikintu icyo ari cyo cyose, genzura icyitegererezo ubwacyo.
Reba ibirango
Emeza:
- kode;
- kode ikomeye;
- nimero y'itsinda;
- gukora cyangwa kurangiza amakuru aho yatanzwe;
- ikigereranyo cyo kuvanga; na
- amabwiriza yo kubika.
Kugenzura isura
Shakisha:
- imyanda itunguranye;
- korohereza;
- ibara rikabije;
- gutandukanya icyiciro;
- kumeneka ibikoresho; cyangwa
- kwanduza.
Ntukibwire ko impinduka zose zigaragara bivuze ko ibicuruzwa bifite inenge, kubera ko sisitemu zimwe na zimwe zishobora gutondeka cyangwa gutuza mu bihe bimwe na bimwe.
Niba isura itandukanye namabwiriza yabatanga, hagarara ubaze mbere yo kwipimisha.
Ikizamini cya 3: Reba imyitwarire ivanze
Umusaruro-mwiza wa epoxy ugomba kuba byoroshye kugereranya no kuvanga buri gihe.
Koresha igipimo nyacyo cyagenwe
Sisitemu ya epoxy ya Veropoxy ntabwo ikoresha igipimo kimwe.
Kurugero, Sisitemu yo gusana & amabara yo kuzamura amabara ikoresha 100: 25 kuburemere, mugihe i Ibara ryongera Epoxy ya Light Granite ikoresha 100: 30 kuburemere.
Ntuzigere ukoresha igipimo kimwe gusa kuberako ibicuruzwa bibiri bisa.
Reba kuvanga uburinganire
Andika niba:
- ibice bibiri bihuza byoroshye;
- imirongo igumaho;
- umwuka mwinshi utangizwa;
- imvange ishyuha vuba; cyangwa
- viscosity ihinduka bidasanzwe mugihe cyo kuvanga.
Kubikorwa bikomeye, koresha uburyo busanzwe bwo kuvanga kugirango buriwese agereranwe neza.
Ikizamini 4: Gupima cyangwa Gereranya Viscosity na Flow
Viscosity nimwe mubintu byingenzi byingirakamaro-igenzura muri epoxy yamabuye.
Ariko ntigomba gufatwa nkamanota yubuziranenge rusange.

Kuki ibicucu bifite akamaro
Iragira ingaruka:
- micro-crack kwinjira;
- gukwirakwiza hejuru;
- mesh;
- vacuum;
- gukoresha resin;
- gutemba; na
- kugumana icyuho.
Gereranya munsi yubushyuhe bumwe
Viscosity ihinduka cyane hamwe nubushyuhe.
Niba Utanga A yapimwe kuri 15 ° C na Supplier B kuri 25 ° C, kugereranya kwawe ni ntege.
Imiterere y'icyitegererezo ku bushyuhe bumwe mbere yo guca urubanza.
Koresha ibizamini byemewe mugihe viscosity ari amasezerano asobanutse
ISO 2555 itanga uburyo busanzwe bwo kuzenguruka kugirango hamenyekane ububobere bugaragara bwibisigazwa byamazi.
ASTM D2196 itanga uburyo bwo kuranga ubwiza bwizunguruka hamwe nimyitwarire ya rheologiya yibikoresho bitari Newtonian.
Kugenzura buri munsi uruganda, ariko, igenzurwa ryikigereranyo cyagereranijwe kirashobora kuba ingirakamaro mugihe ubushyuhe bumwe, ubwinshi, substrate, nigihe cyagenwe.
Ikizamini 5: Gupima ubuzima bwinkono nigihe cyakazi cyingirakamaro
Ntukitiranya ubuzima bwinkono nigihe cyo gukora.
Ubuzima bw'inkono buvuga igice cyinkuru
Epoxy ivanze irashobora kuguma isukuye muri kontineri mugihe imaze kuba ndende cyane kugirango micro-crack yinjira.
Kubitunganya amabuye, igihe cyakazi cyakazi kigomba gusobanurwa na progaramu.
Urugero:
- Ni ryari gucengera kugabanuka kugabanuka kugaragara?
- Ni ryari mesh iba igoye gutose?
- Ni ryari umuvuduko wa vacuum utinda cyane?
- Ni ryari gukwirakwiza hejuru biba bitaringaniye?
Koresha ingano yukuri
Igikombe cya laboratoire 100 g gishobora kwitwara gitandukanye na kg 5 yumusaruro kuko gukiza epoxy irekura ubushyuhe.
Imbaga nini irashobora kugumana ubushyuhe bwinshi kandi ikagabanya ubuzima bwinkono.
Ikizamini 6: Suzuma Umuti Ukiza
“Byarakomeye” ntibihagije.
Uruganda rugomba gusobanukirwa iyo epoxy igeze kubikorwa bitandukanye.
Andika igihe cyo gukora
Ni ryari icyapa gishobora kuba umutekano:
- yazamuye;
- yarahindutse;
- byegeranye;
- yimukiye mu igare;
- yoherejwe kuri kalibrasi; cyangwa
- yoherejwe kuri polishing?
Reba neza umuti utuzuye
Ibimenyetso byo kuburira birimo:
- ubunebwe;
- ahantu hasanwa;
- ibikoresho byoroshye mukibazo;
- gusiga mugihe cyo gusya;
- impumuro idasanzwe nyuma yo gukira; cyangwa
- ubukana butandukanye hagati y'ibice.
Kwipimisha muri laboratoire birashobora kujya kure
Kubushobozi buhanitse bwo gutanga isoko, Calorimetry itandukanye yo gusikana irashobora gukoreshwa mukuranga imyitwarire nigipimo cyo guhinduka mubihe byasobanuwe.
ISO 11357-5 itanga urwego rusanzwe rwa DSC kugirango hamenyekane ubushyuhe bwibihe, ibihe byitwara, ishyaka, nintera yo guhinduka.
Ubu bwoko bwa laboratoire ni ingirakamaro mu kwemeza tekinike ariko ntibikenewe kuri buri ruganda rusanzwe.
Ikizamini 7: Suzuma Kwinjira ku Kibuye gifatika
Iki nikimwe mubizamini byingenzi kuri epoxy yamabuye kandi nikimwe kigoye gusimbuza amakuru rusange ya laboratoire.
Koresha inenge zihagarariye
Ikizamini ku byukuri:
- uduce duto duto;
- ibice bisanzwe;
- fungura imyenge;
- granite yuzuye;
- marble yoroshye; cyangwa
- icyapa cya vacuum.
Ntugacire urubanza kwinjira uhereye hejuru
Icyapa kibengerana cyuzuye ntakintu nakimwe kijyanye no kwinjira imbere.
Nyuma yo gukira, genzura ibice byaciwe, uturere two ku nkombe, kuvunika guhagarariwe aho bikenewe, cyangwa ubundi buryo bwemewe bwo gusuzuma imbere.
Reba nanone kurenza urugero
Kwinjira cyane ntabwo buri gihe ari byiza.
Kuri marble yera yera, kwinjira cyane birashobora gutuma habaho halos yijimye cyangwa ihinduka ryiza rya optique.
Kuri iyo porogaramu, igenzurwa ryinjira rishobora kuba rirenze uburebure bwimbitse.
Ikizamini 8: Reba Guhindura Ibara, Umuhondo ningaruka nziza
Iki kizamini ni ngombwa kuri marble yera, granite yoroheje, onigisi, n'amabuye asobanutse.
Ifoto mbere na nyuma yumucyo ugenzurwa
Koresha itara rimwe, inguni ya kamera, hamwe nubuso.
Amafoto ya terefone yafatiwe mubyumba bitandukanye nibimenyetso bibi.
Tandukanya umuhondo nyawo nigicucu
Agace kijimye gakikije akavuyo karashobora guturuka mubisumizi aho kuba umuhondo wimiti.
Ibi nibyingenzi kuko guhindura epoxy isobanutse ntabwo byanze bikunze bikemura ikibazo kirenze.
Veropoxy's Ntabwo Umuhondo Epoxy ya Hard Marble Yera ihagaze neza cyane igenzurwa no kwinjira cyane kandi umuhondo muke kubibara-amabara.
Tekereza gusaza kubikorwa byimishinga
Niba ibuye rizashyirwa hafi yizuba ryinshi cyangwa niba igihe kirekire cyo kubona neza ari ingenzi, kwihuta kwa UV cyangwa kugereranya ubushyuhe birashobora gufasha urutonde rwabakandida.
Ntugasobanure gusaza byihuse nkubuhanuzi nyabwo bwubuzima bwa serivisi keretse uburyo bwo gukora ikizamini bushigikira uwo mwanzuro.
Ikizamini 9: Suzuma uburyo bwo Kunanirwa no Kunanirwa
"Gukomera gukomeye" nimwe mubisabwa epoxy yo kwamamaza.
Uruganda rwumwuga rugomba kureba uburyo inkwano yananiwe.
Kunanirwa gufatana
Niba epoxy itandukanijwe neza nubuso bwamabuye, intera irashobora kuba idakomeye.
Kunanirwa hamwe
Niba kunanirwa bibaye imbere muri resin yakize, guhuza na substrate birashobora gukomera kuruta imbaraga zimbere muri resin.
Kunanirwa kw'amabuye
Niba ibuye rivunitse mugihe ibifatika bigumye bifatanye, substrate irashobora kuba igice cyintege nke ziteraniro.
Iri tandukanyirizo rirashobora gutanga amakuru arenze umubare wimbaraga mbisi.
Ibizamini byemewe bifatika bifite ihererekanyabubasha
ISO 4587 isobanura igeragezwa rya lap-shear kubiterane bikomeye.
ASTM C882 isuzuma imbaraga za epoxy inkomezi muburyo bugaragara.
Ubu buryo burashobora kumenyesha imitekerereze ya laboratoire, ariko ntanubwo bigomba guhita bifatwa nkibipimo rusange / byananiranye kuri marble cyangwa granite epoxy itabanje kwemeza ko ikurikizwa.
Kubuye risanzwe, igishushanyo mbonera kigomba kwerekana substrate nyayo nuburemere bwimiterere.
Ikigeragezo 10: Reba Gukomera - Ariko Ntukoreshe Gukomera nka Shortcut ya Byose
Epoxy yakize igumye yoroshye muburyo butunguranye irashobora gutera ibibazo cyangwa kuramba.
Igeragezwa rya Durometero rirashobora gutanga ibipimo byerekana umusaruro-kugenzura.
ISO 868 isobanura ibizamini byo gukomera kuri plastike ukoresheje uburyo bwa durometero.
Ariko gukomera byonyine ntibigaragaza gukomera, gukomera, kwinjira, cyangwa kuramba.
Epoxy ikomeye cyane irashobora guhuza nabi amabuye.
Koresha ubukana nka metero imwe ya QC, ntabwo ari umwanzuro wanyuma.
Ikigeragezo 11: Koresha Urusyo nyarwo na Polishinge
Aha niho laboratoire nyinshi itunganijwe neza.
Epoxy yamabuye ni igice cya sisitemu yo gukora.
Niba icyapa kizarangizwa neza, ikigeragezo cyujuje ibisabwa gikeneye guswera.

Reba ibisohoka
Ibisigarira byoroshye cyangwa bidahujwe neza birashobora gukurwa mubice mugihe cyo gusya.
Reba gusiga
Ibikoresho bidakize birashobora gusiga hejuru yamabuye.
Reba neza gloss
Agace kasanwe ntigomba gukora ibishishwa bigaragara neza, imisozi yazamuye, cyangwa isura itandukanye keretse iyo igenewe kubimwemerera.
Reba pinholes nyuma yo gusya
Ubuvuzi bwo hejuru burashobora kugaragara neza mbere yo gusya no kwerekana pinholes nyuma yibintu byakuweho.
Niyo mpanvu icyapa cya nyuma gisizwe - ntabwo ari epoxy itose - nigicuruzwa nyacyo.
Ikizamini 12: Gupima ikoreshwa rya resin
Iki nikimwe mubizamini byingenzi byubucuruzi kandi nikimwe mubirengagizwa.
Kugura igiciro kuri kilo ntabwo bikubwira ikiguzi kuri plaque yarangiye.
Andika garama cyangwa kilo kuri buri cyapa
Koresha umunzani.
Ntugereranye uhereye kumafaranga asigaye mu ndobo.
Gereranya igiciro kuri metero kare
Niba Epoxy A igura 10% munsi yikiro ariko ikoresha ibikoresho 25%, birashobora kuba amahitamo ahenze cyane.
Shyiramo ikiguzi cyo gukora
Igiciro nyacyo gikwiye gutekereza:
- gukoresha epoxy;
- umurimo;
- gukiza gutinda;
- yanze;
- kongera gusya;
- ibisate bimenetse; na
- yatakaje igihe cyo gukora.
Ikizamini 13: Subiramo Ikigeragezo Mubihe Byubushyuhe
Icyitegererezo cyemewe mubushyuhe bumwe bwicyumba gishobora kunanirwa ibihe.
Ubukonje
Ubushyuhe bwo hasi muri rusange:
- kongera ububobere budashidikanywaho;
- kugabanya umuvuduko;
- kwinjira buhoro;
- kwagura gukira; na
- Guhindura igihe.
Ibihe bishyushye
Ubushyuhe bwo hejuru muri rusange:
- kugabanya ubwiza bwambere;
- kongera umuvuduko;
- kwihutisha reaction;
- kugabanya igihe cyo gukora; na
- ongera ibyago bya exothermic mubice byinshi.
Ku nganda zifite ibihe byinshi bitandukanye, uwabitanze arashobora gukenera gusaba sisitemu zitandukanye.
Veropoxy, kurugero, kuri ubu itanga itandukaniro ubushyuhe buke na sisitemu yo hejuru-mesh-sisitemu.
Ikizamini 14: Suzuma Batch-to-Batch Guhuza
Icyitegererezo kimwe cyuzuye ntabwo cyujuje ibyangombwa.
Umusaruro mwinshi biterwa no gusubiramo.
Kuki guhuzagurika bifite akamaro
Itandukaniro hagati yicyiciro rirashobora guhinduka:
- ubwiza;
- igihe cyo gukora;
- gukiza umuvuduko;
- ibara;
- kwinjira;
- gukoresha resin; na
- imyitwarire myiza.
Ntukemere utanga isoko ukurikije icyitegererezo cyateguwe n'intoki
Byiza, impamyabumenyi igomba gutera imbere mubyiciro:
Laboratoire cyangwa ntoya sample trial igeragezwa ryuruganda order gahunda yo kugerageza order gutumiza byinshi.
Ibi biha umuguzi amahirwe yo kureba niba ibicuruzwa byubucuruzi byerekana umusaruro wicyitegererezo.
Ni bangahe ugomba kugerageza?
Nta mubare rusange uhari kuko ibyago biterwa no kubishyira mu bikorwa, agaciro k'amabuye, uburyo bwo guhinduka, n'ubunini bwa gahunda.
Ariko icyapa kimwe ni gake gihagije.
Koresha ingero nyinshi zihagarariye
Impamyabumenyi ifatika igomba gushiramo itandukaniro nka:
- icyapa cyinshi;
- ibisate byinshi;
- ibisate hamwe na micro-crack;
- ibisate bifite inenge nini;
- amabara atandukanye cyangwa imitsi; na
- bisanzwe umusaruro-mwiza wibikoresho, ntabwo byintangarugero gusa.
Nibiciro byinshi byo gutsindwa, gahunda yubushobozi igomba gukomera.
Epoxy Resin Uruganda rwujuje ibyangombwa
| Agace k'ibizamini | Ibyo Kwandika | Igitekerezo cyuruganda |
|---|---|---|
| Inyandiko | TDS, SDS, code yibicuruzwa, amakuru yicyiciro | Wange niba umwirondoro wibanze udasobanutse |
| Kuvanga | Ikigereranyo cyukuri, uburinganire, kumenyekanisha ikirere | Ugomba gusubirwamo nabakozi basanzwe |
| Viscosity / Flow | Temba ku bushyuhe bugenzurwa | Ugomba guhuza kwinjira cyangwa kuzuza porogaramu |
| Igihe cyo gukora | Idirishya ryingirakamaro | Ugomba kurenza igihe nyacyo cyibikorwa hamwe nintera yumutekano |
| Umuti | Gukemura no gutunganya neza | Ugomba guhuza umusaruro |
| Kwinjira | Ubujyakuzimu n'uburinganire | Ugomba kugera ku nenge zisabwa nta kwimuka gukabije |
| Guhindura amabara | Umuhondo, irangi, igicucu | Ugomba kuba wujuje ibisabwa byamabuye |
| Kwizirika | Guhuza imbaraga nuburyo bwo gutsindwa | Ntabwo gutsindwa kwimbere bitemewe |
| Gukomera | Ugereranije ukize gukomera | Nta turere tworoshye cyangwa duhuye |
| Kuringaniza | Gloss, pinholes, gusiga, gukuramo | Gusana birangiye bigomba kwemerwa mubucuruzi |
| Gukoresha | kg / icyapa cyangwa g / m² | Ugomba kuzuza intego |
| Igihagararo cyigihe | Ibigeragezo bikonje kandi bishyushye | Ugomba gukomeza kugenzurwa umwaka wose |
| Guhuriza hamwe | Ubufindo bwinshi cyangwa gahunda yo kugerageza | Ibisubizo bigomba gusubirwamo |
Ibendera ritukura mugihe cya Epoxy itanga isoko
Utanga isoko ntashobora gutanga igipimo kigaragara cyo kuvanga
Iki nikintu cyibanze gisabwa muburyo bwa sisitemu ebyiri.
Viscosity itangwa idafite imiterere yingirakamaro
Umubare wa CPS wambaye ubusa ntabwo uhagije kubigereranya bikomeye.
Buri buye risabwa gukoresha epoxy imwe
Icyatsi cyinshi cya granite, yoroshye ya marble yera, inyuma ya mesh, hamwe na vacuum infusion ntabwo bisabwa gutunganya kimwe.
Utanga isoko abuza kwipimisha icyitegererezo
Kugura byinshi mu nganda, ibi bigomba kubyutsa ibibazo.
Icyitegererezo gikora neza gusa mubihe bigenzurwa nabatanga isoko
Ibikoresho bigomba gukora mu ruganda rwawe, ntabwo muri laboratoire yabatanga gusa.
Utanga isoko akemura ikibazo cyose muguhindura igipimo cya A: B.
Ubushyuhe, ubukonje, umuvuduko ukiza, no kwinjira bigomba kugenzurwa hakoreshejwe uburyo bukwiye hamwe nuburyo bukoreshwa - ntabwo ari impinduka zisanzwe.
Ntamuntu ushobora gusobanura icyitegererezo cyatsinzwe
Inkunga ya tekiniki ifite akamaro cyane mugihe hari ibitagenda neza.
Umuntu utanga isoko agomba gufasha gutandukanya kunanirwa kwibicuruzwa bitagereranijwe, ubushyuhe, kwanduza, ikosa ryo gusaba, cyangwa ibuye ridakwiye.
Nigute wagereranya abatanga Epoxy Babiri
Ntugerageze Utanga A kumurongo umwe mugitondo na Supplier B kumabuye atandukanye nyuma yiminsi itatu.
Koresha ingero zamabuye zihuye
Aho bifatika, gabanya kugereranya ingero zivuye kumurongo umwe cyangwa ibikoresho bihuye neza.
Kugenzura ubushyuhe
Komeza resin, gukomera, n'amabuye muburyo bumwe bwo kugerageza.
Koresha igipimo gikwiye kuri buri gicuruzwa
Kugereranya neza ntabwo bivuze guhatira ibicuruzwa byombi gukoresha igipimo kimwe cyo kuvanga.
Buri gicuruzwa kigomba gutegurwa ukurikije ibisobanuro byacyo.
Koresha intego zingana zo gusaba
Niba ikizamini ari penetration, gereranya kwinjira.
Niba ikizamini ari mesh inyuma, gereranya imikorere mesh.
Ntugashyire urutonde rwa epoxy irwanya ikariso yuzuye ikoresheje amanota rusange.
Kubaka Urutonde Rwikigereranyo Hagati yicyitegererezo nubuguzi bwuzuye
Kubisobanuro byinganda bifite akamaro, akenshi hariho intambwe yo hagati yingirakamaro hagati yicyitegererezo gito cyubusa hamwe nubuguzi bwa kontineri.
Iyo ntambwe nicyemezo cyiburanisha.
Kuki icyemezo cyo kuburanisha gifite akamaro
Ifasha abaguzi gusuzuma:
- gupakira ibicuruzwa;
- icyiciro gihamye;
- gutunganya ububiko;
- umukoresha wiga umurongo;
- ibicuruzwa biva mu mahanga;
- ikoreshwa rya resin;
- ihindagurika ryiza mubisate byinshi; na
- ibikoresho byo gutanga ibikoresho.
Urugero rwa kg 1 ya laboratoire irashobora kwerekana guhuza.
Ntishobora kwerekana byimazeyo umusaruro-mwinshi.
Icyifuzo: Emeza inzira, ntabwo ari ibicuruzwa gusa
Porogaramu nziza ya epoxy yujuje ibisabwa ntabwo ibaza gusa niba resin yujuje urupapuro rwa tekiniki.
Barabaza niba inzira yumusaruro yose isubirwamo.
Niba viscosity ari ukuri ariko abayikora ntibashobora kurangiza icyapa mbere ya gelation, sisitemu ntabwo yujuje ibyangombwa.
Niba gufatana gukomera ariko marble yera ikura halos igaragara, sisitemu ntabwo yujuje ibisabwa kuri iryo buye.
Niba resin ikora neza mugihe cyizuba ariko igahagarika umurongo mugihe cyitumba, inzira yumwaka ntabwo yujuje ibyangombwa.
Niba epoxy ihendutse isaba ibintu byinshi kuri metero kare, gereranya igiciro cyarangiye aho kugura igiciro.
Niba icyitegererezo kimwe gikora ariko ibyiciro byubucuruzi biratandukanye, genzura iperereza kubitanga mbere yo kwiyemeza.
Niba kandi epoxy yatsinze ibizamini bya laboratoire ariko bikananirana mugihe cyo gusya, bizere icyapa cyarangiye.
Umukiriya wawe agura ibuye ryuzuye - ntabwo ari urupapuro rwamakuru.
Ibibazo Bikunze Kubazwa Kubijyanye no Kugerageza Epoxy Mbere yo Gutumiza Byinshi
1. Ni iki uruganda rwamabuye rugomba kugerageza mbere yo kugura epoxy resin kubwinshi?
Uruganda rwamabuye rugomba gusuzuma inyandiko, kuvanga imyitwarire, ubukonje, igihe cyakazi, gukiza, kwinjira, gufatira hamwe, gutuza amabara, gukora neza, gukoresha resin, gukora ubushyuhe bwibihe, no guhuza icyiciro. Ibizamini bigomba gukoresha ibuye ryakozwe kandi rigatunganywa igihe cyose bishoboka.
2. TDS itanga isoko irahagije kugirango yemeze epoxy?
Oya. TDS ni ngombwa mu gusobanukirwa ibyateganijwe no kugeragezwa, ariko ntishobora guhanura neza imikorere kuri buri marble, granite, onyx, cyangwa ibuye ryakozwe. Koresha amakuru ya tekiniki kugirango uhitemo ibicuruzwa, hanyuma wemeze imikorere ukoresheje ibigeragezo byuruganda.
3.Ibisate bingahe bigomba kugeragezwa mbere yo gutumiza byinshi?
Nta mubare rusange. Igisate kimwe mubisanzwe ntabwo gihagije kuko ibuye risanzwe riratandukanye. Gerageza ibyapa byinshi bihagarariye bikubiyemo itandukaniro risanzwe mubyifuzo, ibice, ibara, nuburyo. Nibiciro byinshi byo gutsindwa cyangwa binini byateganijwe, niko gahunda yujuje ibyangombwa igomba kuba ikomeye.
4. Ni ikihe kizamini gikomeye cya epoxy yo gutunganya amabuye?
Nta kizamini kimwe cyingenzi kuri buri porogaramu. Kubisana granite yo gusana, kwinjira birashobora kuba ingenzi. Kuri marble yera, amabara atuje hamwe no kugenzura kwinjira bishobora kuganza. Kubishyigikira mesh, guhanagura no gukemura ikibazo cyo gukiza. Kuri vacuum infusion, viscosity stabilite hamwe nigihe cyo gukora ni ngombwa. Gerageza ukurikije ingaruka zibyara umusaruro.
5. Uruganda rukwiye gushyira itegeko ryikigereranyo mbere yo kugura epoxy yuzuye?
Kubijyanye ninganda zingirakamaro, gahunda yo kugerageza akenshi ni intambwe yo hagati yubwenge. Iyemerera uruganda gusuzuma ibyiciro byubucuruzi, gupakira, guhuza ibikorwa, gukoresha ibicuruzwa, ibicuruzwa biva mu mahanga, imyitwarire yigihe, hamwe nubwizerwe bwabatanga mbere yo kwiyemeza kugura byinshi.
Nigute wahindura icyitegererezo cya Epoxy mubyemezo byizewe byo kugura
Ikizamini cyiza cya epoxy kigomba kubyara ibihe byerekana intsinzi muruganda rwawe. Tekiniki ya tekiniki niyo ntangiriro, ariko icyemezo cya nyuma kigomba gushingira kumabuye nyayo, ubushyuhe nyabwo, igihe nyacyo cyo gusaba, inzira nyayo yo kurangiza, hamwe nigiciro cyapimwe cyumusaruro. Ikigamijwe ntabwo ari ugushaka ibisigazwa bikora rimwe-ni ukwemeza inzira isubirwamo ishobora kugabanuka neza mubicuruzwa byubucuruzi.
Gerageza ukurikije ingaruka zo gusaba
Granite micro-crack gusana:
shyira imbere ubujyakuzimu, igihe cyakazi, gukiza, hamwe nigisubizo.
Marble yera:
shyira imbere umuhondo, gusiga, kugicucu, kugenzura kwinjira, no kugaragara neza.
Gushyigikira Mesh:
shyira imbere fibre fibre, gufatisha amabuye, igihe cyakazi, gukemura gukira, nubushyuhe bwibihe.
Kwinjiza Vacuum:
shyira imbere ubukonje buke-buke, idirishya ryinjizwamo, ibituba, ibyiyumvo bitemba, kwinjira, hamwe no gukoresha resin.
Kuzuza ikiziba no kuziba:
shyira imbere kugenzura imigendekere, gutuza kurwego, kugumana hejuru, imyitwarire ya polishinge, hamwe nu mukino ugaragara.
Ntukemere icyitegererezo kidafite imibare
"Birasa neza" biragoye kubyara. Andika resin hamwe na numero yicyiciro, A: B igipimo, ubushyuhe, ingano yicyiciro, igihe cyakazi, gukiza igihe, gukoresha resin, kwitegereza kwangwa, nibisubizo bya polishing. Ndetse ikizamini cyoroheje cyuruganda kiba ingirakamaro cyane mugihe undi mukoresha ashobora kugisubiramo akoresheje ibintu bimwe.
Gereranya agaciro k'umusaruro wose, ntabwo igiciro kuri kilo gusa
Epoxy ihenze cyane irashobora kubahendutse mubikorwa iyo igabanije gukoresha, gukiza gutinda, ibisate bimenetse, kongera gusya, cyangwa kwanga. Ibinyuranye, ibicuruzwa bitangaje bya tekiniki birashobora kuba bidakwiriye ubucuruzi mugihe cyigihe cyacyo cyangwa ibisabwa byabakozi bidahuye nuruganda. Suzuma igiciro kuri plaque yemewe irangiye kuruta igiciro cyingoma wenyine.
Niki gitandukanya utanga isoko ningirakamaro kugurisha ibicuruzwa?
Utanga isoko yingirakamaro agomba gufasha gusobanura sisitemu yukuri ya resin-gukomera, gusobanura ibipimo bya tekiniki, gushyigikira ikigereranyo cyikigereranyo, gukora iperereza ryatsinzwe, gusaba ihinduka ryigihe aho bibaye ngombwa, no gukomeza ibyiciro byubucuruzi bihoraho. Ku baguzi binganda, inkunga ya tekiniki nyuma yikizamini cyatsinzwe irashobora kuba iyagaciro kuruta icyitegererezo cyiza cyo kugurisha.
Icyifuzo gifatika
Sobanura ibyago byo gutsindwa mbere, hanyuma wubake icyitegererezo cyikikije. Koresha ibuye ryawe bwite, upime inzira, usige cyangwa ukoreshe icyapa neza nkuko umusaruro ubisaba, subiramo igeragezwa mubice byinshi byerekana, kandi ugereranye ibyo ukoresha byose kandi wange ingaruka. Niba icyitegererezo cyatsinzwe, jya kumurongo wateganijwe mbere yo kwiyemeza kugura byinshi. Kugura epoxy yizewe ntabwo bishingiye ku gatabo keza-gashingiye ku bisubizo by'uruganda rusubirwamo.
Witegure Kugerageza Epoxy Kumabuye Yawe Mbere yo Gutumiza Byinshi?
Sangira ubwoko bwibuye, imiterere yubushuhe, ubushyuhe bwamahugurwa, ikibazo cya epoxy yubu, uburyo bwo gusaba, hamwe nibisabwa byingirakamaro. Ikigeragezo cyuruganda ukoresheje icyapa gihagarariwe kirashobora gufasha gusuzuma kwinjira, gukira, gutuza amabara, gusiga, gukoresha, no guhuza ibikorwa mbere yo kugura byinshi.
Reba
- Umuryango mpuzamahanga ushinzwe ubuziranenge.
ISO 25.
ISO / TC 61.
Umuryango mpuzamahanga ushinzwe ubuziranenge. - ASTM Mpuzamahanga.
ASTM D2196-20 (2026) - Uburyo Bwipimisha Bwuburyo Bwiza bwa Rheologiya Ibikoresho bitari Newtonian by Rotational Viscometer.
Komite ya ASTM D01.
ASTM International, 2026. - Umuryango mpuzamahanga ushinzwe ubuziranenge.
ISO 11.
ISO/TC 61/SC 5.
International Organization for Standardization, 2025. - Umuryango mpuzamahanga ushinzwe ubuziranenge.
ISO 868: 2003 - Plastike na Ebonite - Kumenya ubukana bwa Indentation hakoreshejwe uburyo bwa Durometero.
ISO / TC 61.
Umuryango mpuzamahanga ushinzwe ubuziranenge. - Umuryango mpuzamahanga ushinzwe ubuziranenge.
ISO 4587: 2003 - Ibifatika - Kugena imbaraga za Tensile Lap-Shear Imbaraga za Rigid-to-Rigid Bonded Assemblies.
ISO / TC 61 / SC 11.
Umuryango mpuzamahanga ushinzwe ubuziranenge. - ASTM Mpuzamahanga.
ASTM C882 / C882M-23 - Uburyo busanzwe bwo gupima uburyo bwo guhuza imbaraga za Epoxy-Resin Sisitemu ikoreshwa na beto na Slant Shear.
Komite ya ASTM C09.
ASTM Mpuzamahanga. - CYIZA SYSTEM Abakozi ba tekinike.
CYIZA SYSTEM Umukoresha Igitabo & Ubuyobozi.
Gougeon Brothers, Inc.
SYSTEM YIZA CYANE. - Charles Selwitz.
Epoxy isubira mu kubungabunga amabuye.
Ikigo cyo Kubungabunga Getty.
Ubushakashatsi muburyo bwo kubungabunga, Getty Publications, 1992.